Material DryingUpdated 2 months ago
| Material | Temperature (°C) | Min Duration (Hrs) | Comments |
| PLA | 65 | 4 | |
| PETG | 65 | 4 | |
| ABS | 85 | 2 | |
| ASA | 85 | 2 | |
| HIPS | 75 | 2 | Drying generally not needed |
| PP | 65 | 2 | Drying generally not needed |
| PE (OBC) | 65 | 2 | Drying generally not needed |
| PCTG | 65 | 2 | |
| TPU | 65 | 4 | |
| PC/ABS | 110 | 4 | |
| PC | 120 | 4 | |
| PA6 | 85 | 4 | |
| PA12 | 85 | 4 | |
| PPA/HTN | 110 | 4 | |
| PPE/PS | 90 | 4 | |
| PVDF | 65 | 4 | Drying generally not needed |
| PPS | 90 | 4 | |
| PSU | 150 | 4 | |
| PES | 150 | 4 | |
| PPSU | 150 | 4 | |
| Ultem 9085 | 140 | 4 | |
| Ultem 1010 | 150 | 4 | |
| PEKK | 140 | 4 | |
| PEEK | 140 | 4 | |
| TPI | 150 | 4 | |
| Victrex AM200 | 120 | 6 | Victrex uses a PC reel |
| LTS1/LTS2 | 75 | 2 | Drying generally not needed |
| MTS2 | 90 | 4 | |
| HTS1 | 150 | 4 | |
| HTS2 | 150 | 4 | |
| PVA | 55 | 4 | |
| X1 USM | 55 | 4 | |
| Note: These temperatures are for 3DX materials wound onto 3DX-provided reels. Other suppliers' materials and reels may be made using materials that cannot withstand these temps. | |||